Heat-shrink tubing after shrinking: wall-thickness and seal verification — sampling, measurement, seal test and disposition
Test scope: what is verified and what is not
This verification covers shrinkage completion, wall thickness, end sealing and appearance; it does not replace electrical continuity, withstand-voltage or connector seal tests. Adhesive-lined and plain tubing have different acceptance rules. Before testing, confirm tube specification, shrink ratio, adhesive type and product specification so that one acceptance card is not applied to every construction.
Sampling: which batch and which sections
Sample from a production batch made with the same tube lot, the same heating equipment and the same parameters, covering the beginning, middle and end of the batch. For each node, take a middle section, a section near the end and an overlap section; the length depends on the measurement and seal test. Samples must be free of scratches, scorch marks and artificial flattening, and the sampling positions and quantity go into the record.
Wall and dimension measurement: points, instruments and judgment
Use a suitable instrument to measure wall thickness at several points around the circumference of the shrunk section, avoiding adhesive build-up and cut edges; also check the outside diameter, length change and whether the end is fully closed. Judge a failure when wall thickness is below the product specification, or when voids, delamination or obvious eccentricity appear; do not rely on the average alone.
Seal test: how to verify an adhesive-lined end
For adhesive-lined tubing, run the end seal test defined by the product specification: a specified-pressure air-tightness test or dye penetration, observing the end, the overlap seam and the adhesive boundary for leakage. Apply the specified pressure and hold time; do not raise pressure to improve the pass rate. Plain tubing is checked only for appearance and wall thickness, without applying the seal criterion.
Disposition and batch handling: how to isolate failures
Accept when all measurement points pass and no leakage appears. Reject when any point is below the lower limit, or voids, delamination, scorch marks or leakage appear. Isolate the failed batch and retest the same batch with doubled sampling. If failures continue, stop the line and trace the tube lot, heating equipment, temperature window and operator. Keep records with the batch record. For the process description, see heat-shrink tubing and shrinking process.