Ultrasonic weld pull and cross-section inspection: sampling, judgment and batch handling
Test boundaries: what pull and cross-section each show
The pull test measures the weld under axial load, and the failure location separates strand breakage from weld separation. The cross-section shows whether fusion is continuous and reveals voids and oxide inclusions. Both tests are required; one alone cannot release a weld.
Sampling: which welds to take
Sample per the control plan from the first piece, after parameter changes, after horn changes and from production lots. Take the same location and wire combination within a lot; samples must not be re-welded or dressed. Follow the specified quantity, location and frequency.
Pull test: fixturing, travel and records
Clamp the harness on both sides of the weld without damaging strands; keep the pull speed stable and record the peak and failure location. A strand break before weld separation is recorded separately from a weld that pulls out as a whole.
Cross-section: preparation and observation
Cut perpendicular to the weld axis, mount, grind and polish before observation. Look for lack of fusion, voids, oxide inclusions, over-weld and flash. File the cross-section image with the weld ID and parameter record.
Judgment and batch: what to do with a failure
Weld separation, lack of fusion, voids or over-weld beyond specification is a reject. Isolate the batch and trace the horn, parameters and wire size. Reworked parts are re-inspected; an abnormal batch is not released directly. For the process, see ultrasonic welding process.